Aluminum alloy heat treatment and quenching process

Date:2020-05-27

Aluminum alloy heat treatment and quenching process

1、Aluminum alloy heat treatment process。

The purpose of this process is to make a large amount of hardening elements that can be used, such as copper, magnesium, zinc, or polydissolved solids, into a solid melt, which must be kept at a high temperature of 535 degrees to 550 degrees for a long enough time. 8 hours, and obtain a more homogeneous solid solution. 1. Aluminum alloy solid solution temperature, aluminum alloy rim solid solution state point is 530 degrees, the melting point is 555 degrees, beyond this temperature begins to melt into aluminum water。

Main points of aluminum alloy heat treatment process:

A.When warming up, first turn on the windmill cooling water first, then turn on the windmill fully to set the operating temperature and combustion status

When entering the furnace (the casting is placed with the A side facing up, and the A side is forbidden (during solution treatment))

B.Solid solution aging treatment conditions 545 degrees * 8H + 130 degrees * 6H The temperature must be stable and uniform, according to the design strength of the rim、

Material, characteristics, testing decision。

C.The quenching water temperature is 60 degrees-80 degrees water temperature, the casting is not easy to deform, and the quenching time is counted from the door to

The uppermost casting is fully soaked in water, and the time is 16 seconds to 20 seconds to complete the instant quenching water。

D.Full inspection items after solution treatment, deformation inspection, reshaping, steel characters to prevent abnormal quality tracking, every time after aging

The hardness of one casting is measured on the upper and lower layers of the trolley, the value is 65-75HB. Cooperating with continuous automatic operation is the same as high temperature operation, enter the furnace after the furnace is pre-fired, and enter and exit the furnace regularly according to the time set by the timer。

2、Delaying process of aluminum alloy quenching water。

When quenching water, the casting is taken from the solution temperature in the furnace to the quenching water. The time it takes is the delay of quenching water. The delay of quenching water is 15 seconds> 18 seconds. The most commonly used quenching liquid is water, and the rest is air or liquid nitrogen, etc., but the stress and distortion caused by quenching should be considered. Sometimes hot water is needed to prevent deformation and cracking. 5. Precipitation hardening When heat-treatable aluminum alloy is quenched to normal temperature, due to the low solubility of solute at low temperature, it produces a saturated and unstable state, so some tissues will precipitate in the base, and the precipitation effect at room temperature is Natural aging, if it needs to be heated to a certain temperature, the precipitation is artificial aging。


分享
×
欧美精品一区二区水蜜桃| 国产成人在线一区二区三区| 一级片二级片欧美日韩| 青青操成人免费在线视频| 国产一区二区三区丝袜不卡| 成人免费观看视频免费| 成人精品网一区二区三区| 欧美中文日韩一区久久| 日韩国产亚洲一区二区三区| 免费观看潮喷到高潮大叫| 国产精品国产亚洲区久久| 国产男女激情在线视频| 99久久人妻中文字幕| 欧美自拍偷自拍亚洲精品| 国产欧美精品对白性色| 国产又粗又猛又长又大| 东京热电东京热一区二区三区| 欧美日韩国产另类一区二区| 成人欧美一区二区三区视频| 午夜福利92在线观看| 不卡免费成人日韩精品| 日本国产欧美精品视频| 黄色av尤物白丝在线播放网址 | 欧美熟妇一区二区在线| 黄色国产自拍在线观看| 中字幕一区二区三区久久蜜桃| 大尺度激情福利视频在线观看| 日韩欧美第一页在线观看| 日本办公室三级在线观看| 精品精品国产欧美在线| 欧美午夜不卡在线观看| 亚洲熟女熟妇乱色一区| 国产成人精品在线一区二区三区| 能在线看的视频你懂的| 91人妻久久精品一区二区三区| 中文字幕日韩无套内射| 久久综合亚洲精品蜜桃| 亚洲另类欧美综合日韩精品| 好吊日成人免费视频公开| 蜜桃传媒在线正在播放| 99福利一区二区视频|